Home / Technical Data
| Grade | C | Si | Mn | P | S | Cr | Ni | Mo |
|---|---|---|---|---|---|---|---|---|
| A2 (304) | 0.08 | 1.00 | 2.00 | 0.045 | 0.030 | 18 – 20 | 8 – 10.5 | – |
| A4 (316) | 0.08 | 1.00 | 2.00 | 0.045 | 0.030 | 16 – 18 | 10 – 14 | 2 – 3 |
Maximum percentages unless a range is shown. Typical values for guidance only.
| Property class | Min. tensile strength | Min. 0.2% proof strength | Condition |
|---|---|---|---|
| 50 | 500 MPa | 210 MPa | Soft |
| 70 | 700 MPa | 450 MPa | Cold-worked |
| 80 | 800 MPa | 600 MPa | Highly cold-worked |
Values for bolts and screws per ISO 3506-1. Confirm against the current standard for your design.
Metal is shaped at room temperature in dies. Used for smaller diameters. Gives tight tolerances, a smooth finish, good grain flow and an efficient process for large volumes.
The bar is heated until soft and then forged. Used for larger diameters where cold forming is impractical. Makes heavy sizes possible, followed by machining and threading.
The maximum pulling stress a fastener can withstand before it breaks.
The stress at which a fastener begins to deform permanently. Stainless fasteners are rated by 0.2% proof strength.
A specified test load a fastener must carry without permanent deformation.
A chemical treatment that removes free iron from the surface and helps the protective chromium oxide film form.
A thin, invisible chromium-rich oxide layer that protects stainless steel from corrosion and self-heals when scratched in air.
Increase in strength and hardness as metal is deformed. Austenitic stainless steels work-harden strongly, which is why cold-forged parts can be stronger.
Annealed austenitic stainless steel is non-magnetic. Cold forming can make it slightly magnetic, which does not mean it is lower in quality.
Seizure of stainless threads under load. Reduce the risk with lubrication, moderate speed when tightening and mixed grades where suitable.